| Specification | AMS 4200 | |||||||
|---|---|---|---|---|---|---|---|---|
| Form | Plate | |||||||
| Temper | T7351 | |||||||
| Thickness, in. | 0.750- 1.000 | 1.001- 1.500 | 1.501- 2.000 | 2.001- 2.500 | 2.501- 3.000 | 3.001- 4.000 | 4.001- 4.500 | 4.501- 5.000 |
| Basis | S | S | S | S | S | S | S | S |
| Mechanical Properties: | ||||||||
| Ftu, ksi: | ||||||||
| L | 72 | 72 | 71 | 70 | 68 | 68 | ||
| LT | 74 | 73 | 73 | 73 | 72 | 70 | 68 | 68 |
| ST | 69 | 69 | 68 | 65 | 63 | 63 | ||
| Fy, ksi: | ||||||||
| L | 64 | 63 | 62 | 60 | 58 | 58 | ||
| LT | 65 | 64 | 64 | 63 | 62 | 60 | 58 | 58 |
| ST | 59 | 58 | 57 | 56 | 54 | 54 | ||
| Fcy, ksi: | ||||||||
| L | 64 | 63 | 62 | 60 | 58 | |||
| LT | 69 | 68 | 67 | 64 | 62 | |||
| ST | 69 | 68 | 67 | 64 | 62 | |||
| Fsu, ksi | 41 | 41 | 41 | 39 | 38 | |||
| Fbru2, ksi: | ||||||||
| (e/D = 1.5) | 114 | 112 | 109 | 106 | ||||
| (e/D = 2.0) | 146 | 144 | 140 | 136 | ||||
| Fbry3, ksi: | ||||||||
| (e/D = 1.5) | 91 | 89 | 86 | 83 | ||||
| (e/D = 2.0) | 106 | 104 | 101 | 97 | ||||
| e, percent: | ||||||||
| L | 6 | 6 | 5 | |||||
| LT | 8 | 8 | 7 | 6 | 6 | 5 | 5 | 5 |
| ST | 2 | 2 | 2 | |||||
| E, 103 ksi | 10.1 | |||||||
| Ec, 103 ksi | 10.4 | |||||||
| G, 103 ksi | 3.9 | |||||||
| μ | 0.33 | |||||||
| Physical Properties: | ||||||||
| ω, lb/in.3 | 0.103 | |||||||
| C, Btu/(lb)(°F) | 0.23 (at 212°F) | |||||||
| K, Btu/[(hr)(ft²)(°F)/ft] | 89 (at 77°F) | |||||||
| α, 10-6 in./in./°F | 13.0 (RT to 212°F) | |||||||
MIL-HDBK-5J
3.7.3.0 (c). Design Mechanical and Physical Properties of 7049/7149 Aluminum Alloy Die Forging
| Specification | AMS-QQ-A-367, AMS 4111, AMS 4320, and AMS-A-22771 | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Form | Die forging | |||||||||
| Temper | T73a | |||||||||
| Thicknessb, in. | ≤1.000 | 1.001-2.000 | 2.001-3.000 | 3.001-4.000 | 4.001-5.000 | |||||
| Basis | A | B | A | B | A | B | A | B | A | B |
| Mechanical Properties: | ||||||||||
| Ftu ksi: | ||||||||||
| L | 71 | 74 | 70 | 73 | 69 | 72 | 68 | 71 | 67 | 70 |
| Tc (S-basis) | 71d | 70d | 70d | 70d | 68d | |||||
| Fty ksi: | ||||||||||
| L | 60 | 64 | 59 | 63 | 58 | 61 | 57 | 60 | 55 | 59 |
| Tc (S-basis) | 61d | 60d | 60d | 60d | 58d | |||||
| Fcy ksi: | ||||||||||
| L | 62 | 66 | 61 | 65 | 60 | 63 | 59 | 62 | 57 | 61 |
| ST | 56 | 60 | 55 | 59 | 54 | 57 | 53 | 56 | 51 | 55 |
| Fsu ksi | 40 | 41 | 39 | 41 | 39 | 40 | 38 | 40 | 37 | 39 |
| Fbru ksi: | ||||||||||
| (e/D = 1.5) | 100 | 105 | 99 | 103 | 98 | 102 | 96 | 100 | 95 | 99 |
| (e/D = 2.0) | 132 | 138 | 130 | 136 | 128 | 134 | 126 | 132 | 125 | 130 |
| Fbry ksi: | ||||||||||
| (e/D = 1.5) | 76 | 82 | 75 | 80 | 74 | 78 | 73 | 76 | 70 | 75 |
| (e/D = 2.0) | 93 | 99 | 91 | 97 | 90 | 94 | 88 | 93 | 85 | 91 |
| e, percent (S-basis): | ||||||||||
| L | 7 | 7 | 7 | 7 | 7 | |||||
| Tc | 3 | 3 | 3 | 3 | 2 | |||||
| E, 10³ ksi | 10.2 | |||||||||
| Ec, 10³ ksi | 10.7 | |||||||||
| G, 10³ ksi | 3.9 | |||||||||
| μ | 0.33 | |||||||||
| Physical Properties: | ||||||||||
| ω, lb/in.³ | 0.103 | |||||||||
| C, Btu/(lb)(°F) | 0.25 (at 212°F) | |||||||||
| K, Btu/[(hr)(ft²)(°F)/ft] | 89 (at 77°F) | |||||||||
| α, 10-6 in./in./°F | 13.0 (RT to 212°F) | |||||||||
- a Design values were based upon data obtained from testing T73 die forgings, heat treated by suppliers and supplied in T73 temper.
- b Thickness at the time of heat treatment. When die forgings are machined before heat treatment, the mechanical properties are applicable provided the as-forged thickness is not greater than twice the thickness at the time of heat treatment.
- c T indicates any grain direction not within ±15° of being parallel to the forging flow lines. Fcy(T) values are based upon short transverse (ST) test data.
- d Specification value. T tensile properties are presented on an S-basis only.
- e Bearing values are "dry pin" values per Section 1.4.7.1.
MIL-HDBK-5J
3.7.3.0 (d). Design Mechanical and Physical Properties of 7049/7149 Aluminum Alloy Hand Forging
| Specification | AMS-QQ-A-367, AMS 4111, AMS 4320, and AMS-A-22771 | ||
|---|---|---|---|
| Form | Hand forging | ||
| Temper | T73 | ||
| Thicknessa, in. | 2.001-3.000 | 3.001-4.000 | 4.001-5.000 |
| Basis | S | S | S |
| Mechanical Properties: | |||
| Fu, ksi: | |||
| L | 71 | 69 | 67 |
| LT | 71 | 69 | 67 |
| ST | 69 | 67 | 66 |
| Fry, ksi: | |||
| L | 61 | 59 | 56 |
| LT | 59 | 57 | 56 |
| ST | 58 | 56 | 55 |
| Fcy, ksi: | |||
| L | 60 | 58 | 57 |
| LT | 61 | 59 | 57 |
| ST | 61 | 59 | 58 |
| Fsu, ksi: | |||
| L | 42 | 41 | 39 |
| LT | 41 | 39 | 38 |
| ST | 41 | 40 | 39 |
| Fbru, ksi: | |||
| (e/D = 1.5) | 102 | 100 | 97 |
| (e/D = 2.0) | 134 | 130 | 126 |
| Fbry, ksi: | |||
| (e/D = 1.5) | 81 | 79 | 77 |
| (e/D = 2.0) | 96 | 92 | 91 |
| e, percent: | |||
| L | 9 | 8 | 7 |
| LT | 4 | 3 | 3 |
| ST | 3 | 2 | 2 |
| E, 103 ksi | 10.2 | ||
| E, 103 ksi | 10.6 | ||
| G, 103 ksi | 3.9 | ||
| μ | 0.33 | ||
| Physical Properties: | |||
| ω, lb./in.3 | 0.103 | ||
| C, Btu/(lb)(°F) | 0.23 (at 212°F) | ||
| K, Btu/[(hr)(ft2)(°F)/ft] | 89 (at 77°F) | ||
| α, 10-6 in./in./°F | 13.0 (RT to 212°F) | ||
a When hand forgings are machined before heat treatment, section thickness at time of heat treatment will determine minimum mechanical properties as long as original (as-forged) thickness does not exceed maximum thickness for the alloy as shown in the table. The maximum cross-section area of hand forgings is 256 sq. in.
b Bearing values are “dry pin” values per Section 1.4.7.1.
MIL-HDBK-5J
3.7.3.0 (e). Design Mechanical and Physical Properties of 7049/7149 Aluminum Alloy Extrusion
| Specification | AMS 4157 and AMS 4343 | ||
|---|---|---|---|
| Form | Extrusion | ||
| Temper | T73511 | ||
| Thickness,ª in. | ≤ 2.499 | 2.500-2.999 | 3.000-5.000 |
| Basis | S | S | S |
| Mechanical Properties: | |||
| Ftu* ksi: | |||
| L | 74 | 74 | 72 |
| LT | 70 | 70 | 68 |
| ST | 70 | 68 | |
| Fty* ksi: | |||
| L | 64 | 64 | 62 |
| LT | 60 | 60 | 58 |
| ST | 60 | 58 | |
| Fcy* ksi: | |||
| L | 65 | 65 | 63 |
| LT | |||
| ST | |||
| Fsu* ksi: | 40 | 40 | 39 |
| Fbbru ksi: | |||
| (e/D = 1.5) | 110 | 110 | 107 |
| (e/D = 2.0) | 144 | 144 | 140 |
| Fbbry ksi: | |||
| (e/D = 1.5) | 85 | 85 | 83 |
| (e/D = 2.0) | 105 | 105 | 101 |
| e, percent: | |||
| L | 7 | 7 | 7 |
| LT | 5 | 5 | |
| ST | 5 | 5 | |
| E, 10³ ksi | 10.5 | ||
| E, 10³ ksi | 11.0 | ||
| G, 10³ ksi | 4.0 | ||
| μ | 0.33 | ||
| Physical Properties: | |||
| ω, lb/in.³ | 0.103 | ||
| C, Btu/(lb)(°F) | 0.23 (at 212°F) | ||
| K, Btu/[(hr)(ft²)(°F)/ft] | 89 (at 77°F) | ||
| α, 10−6 in./in./°F | 13.0 (RT to 212°F) | ||