9Ni-4Co-0.30C Steel
| Specification | Form |
|---|---|
| AMS 6524a | Sheet, strip, and plate |
| AMS 6526 | Bar, forging, and tubing |
a Noncurrent specification.
2.4.3.1 Heat-Treated Condition — Effect of temperature on various mechanical properties is presented in Figures 2.4.3.1.1. through 2.4.3.1.4. Typical stress-strain and tangent-modulus curves are presented in Figures 2.4.3.1.6(a) through (d). Notched fatigue data at room temperature are illustrated in Figure 2.4.3.1.8.
Downloaded from https://www.everyspec.com MIL-HDBK-5J
2.4.3.0 (b). Design Mechanical and Physical Properties of 9Ni-4Co-0.30C Steel
| Specification | AMS 6524a | AMS 6526 | |
|---|---|---|---|
| Form | Sheet, strip, and plate | Bar, forging, and tubing | |
| Condition | Quenched and tempered | Quenched and tempered | |
| Thickness, in. | ≤0.249 | ≥0.250 | <4.000 |
| Basis | Sb | Sb | Sb |
| Mechanical Properties: | |||
| Ftu, ksi: | |||
| L | 220 | ||
| LT | 220 | 220 | |
| Fty, ksi: | |||
| L | 190 | ||
| LT | 185 | 190 | |
| Fcy, ksi: | |||
| L | 209 | ||
| LT | 209 | ||
| Fsu, ksi | 137 | 137 | |
| Fbruc, ksi: | |||
| (e/D = 1.5) | 346 | 346 | |
| (e/D = 2.0) | 440 | 440 | |
| Fbry, ksi: | |||
| (e/D = 1.5) | 291 | 291 | |
| (e/D = 2.0) | 322 | 322 | |
| e, percent: | |||
| L | 10 | ||
| LT | 6 | 10 | |
| RA, percent: | |||
| L | 40 | ||
| LT | 35 | ||
| E, 103 ksi | 28.5 | ||
| Ec, 103 ksi | 29.8 | ||
| G, 103 ksi | |||
| μ | |||
| Physical Properties: | |||
| ω, lb/in.3 | 0.28 | ||
| C, Btu/(lb)(°F) | |||
| K, Btu/[(hr)(ft2)(°F)/ft] | 13.3 (75°F) | ||
| α, 10-6 in./in./°F | See Figure 2.4.3.0 | ||